Chemical etching removes metal by dissolving it, so the design rules differ from machining in predictable ways. Most etching problems trace back to a feature that is too small for the sheet thickness, or to an undercut that was not compensated in the artwork.

How the process works

  1. Clean the sheet and laminate a photoresist on both sides.
  2. Expose the resist through a phototool carrying the part pattern.
  3. Develop the resist so the areas to be etched are exposed.
  4. Etch in a controlled chemical bath until the depth is reached.
  5. Strip the resist, then inspect and finish the parts.

Core design rules

FeatureRule of thumbNotes
Minimum line width0.07mm standard, 0.02mm achievableUltra-thin sheet below 0.05mm allows finer lines
Minimum hole diameterClose to 1x sheet thicknessAspect ratio up to 1.5:1 on thin stock
Minimum spacingAt least 1x sheet thicknessTighter spacing risks the web breaking
Corner radiusAt least 1x thickness on internal cornersSharp internal corners etch unevenly
UndercutAbout 1.2 - 1.5x thickness per sideCompensate in the artwork for critical dimensions
Tie bars0.2 - 0.5mm wide, added during etchingKeep parts attached to the sheet until assembly

Understanding undercut

Etching works sideways as well as downwards, so the cut edge curves inward. This is called undercut and it grows with etch depth. For a part with a critical outer dimension, the artwork is pre-compensated by the expected undercut so the finished part lands on nominal size. When a drawing gives only the final dimension, ask the etcher to confirm the compensation rather than assuming the artwork is literal.

Materials that etch well

  • Stainless steel 304, 316L and 430, the most common etching materials.
  • Copper, brass and beryllium copper for contacts, shields and antennas.
  • Aluminum, which needs a different chemistry and tighter process control.
  • Titanium, Kovar and nickel alloys for medical and electronic parts.
  • Thin spring steel for reeds, clips and shutter blades.

What affects the tolerance

Tolerance depends on sheet thickness, feature size and whether the dimension crosses the etch direction. A ±0.01mm band is realistic on thin sheet with moderate features. On a 0.5mm part with a 0.05mm slot, the same process may drift to ±0.02mm. Etching both sides at once halves the undercut error compared with single-sided etching, which is why double-sided etching is standard for precision parts.

Common design mistakes

  • Specifying a hole smaller than the sheet thickness without accepting a tapered wall.
  • Leaving a zero-radius internal corner that the etchant cannot reproduce.
  • Placing features so close that the web between them breaks during handling.
  • Forgetting tie bars, so parts fall free in the bath and are lost.
  • Dimensioning to a sharp edge instead of allowing for undercut.
What is the minimum hole size in chemical etching?
The practical rule is a hole diameter close to the sheet thickness, up to an aspect ratio of about 1.5:1 on thin material. A 0.05mm hole in 0.03mm sheet is achievable, while the same hole in 0.2mm sheet is not.
Does etching leave burrs?
No. The process dissolves metal rather than shearing it, so there is no burr and no need for a deburring step.
Do I need a hard tool for etching?
No hard tool is required. A phototool is generated from your CAD file, and it is reused for repeat orders of the same design.

Have drawings? Send them over, reply within 10 minutes

Send your CAD file and we will review the design against etching rules before quoting, so problems are caught before production.

Send Drawings · Free Quote

Related Technical Articles

Send your drawings, get a preliminary quote within 10 minutes

Supports CAD / PDF / DXF / STEP. Specify material, thickness and quantity. Free process evaluation from our engineers.

📞 📝 📍
🏠Home📞Call✉Quote